The Differences Between Heat-Treatable and Non-Heat-Treatable Aluminum Alloys

Print Print

By: Tony Anderson CEng.

Q - I have often heard the terms Heat-Treatable and Non-Heat-Treatable Aluminum Alloys.  What are the differences between these alloys, and how does the type of base alloy affect the final strength of the weld?

A - Heat-Treatable and Non-Heat-Treatable are the two basic types of aluminum alloys.  They are both widely used in welding fabrication and have somewhat different characteristics associated with their chemical and metallurgical structure and their reactions during the arc welding process.

In order to best answer your question, we first need to understand the basic differences between these two groups of alloys.

Non-Heat-Treatable Aluminum Alloys - The strength of these alloys is initially produced by alloying the aluminum with additions of other elements.  These alloys consist of the pure aluminum alloys (1xxx series), manganese alloys (3xxx series), silicon alloys (4xxx series) and magnesium alloys (5xxx series).  A further increase in strength of these alloys is obtained through various degrees of cold working or strain hardening.  Cold working or strain hardening is accomplished by rolling, drawing through dies, stretching or similar operations where area reduction is obtained.  Regulating the amount of total reduction in area of the material controls its final properties.  Material which has been subjected to a strain-hardening temper, may also be given a final, elevated temperature treatment called “stabilizing”, to ensure that the final mechanical properties do not change over time.

The letter “H” followed by numbers denotes the specific condition obtained from strain hardening.

The first number following the “H” indicates the basic operations used during or after strain hardening:

H1 – Strain hardened only

H2 – Strain hardened and partially annealed

H3 – Strain hardened and stabilized

The second number following the “H” indicates the degree of strain hardening:

HX2 – Quarter Hard

HX4 – Half Hard

HX6 – Three-Quarter Hard

HX8 – Full Hard

HX9 – Extra Hard

Heat-Treatable Aluminum Alloys - The initial strength of these alloys is also produced by the addition of alloying elements to pure aluminum.  These elements include copper (2xxx series), magnesium and silicon, which is able to form the compound magnesium silicide (6xxx series), and zinc (7xxx series).  When present in a given alloy, singly or in various combinations, these elements exhibit increasing solid solubility in aluminum as the temperature increases.  Because of this reaction, it is possible to produce significant additional strengthening to the heat-treatable alloys by subjecting them to an elevated thermal treatment, quenching, and, when applicable, precipitation heat-treatment known also as artificial aging.

Note:  Because of additions of magnesium and or copper, there are also a number of silicon (4xxx series) alloys that are heat-treatable.

In solution heat-treatment, the material is typically heated to temperatures of 900 to 1050 deg F, depending upon the alloy.  This causes the alloying elements within the material to go into solid solution.  Rapid quenching, usually in water, which freezes or traps the alloying elements in solution, follows this process.

Precipitation heat-treatment or artificial aging is used after solution heat-treatment.  This involves heating the material for a controlled time at a lower temperature (around 250 to 400 deg F).  This process, used after solution heat-treatment, both increases strength and stabilizes the material.

How does the type of material, heat-treated or non-heat-treated, affect the completed strength of the weld?

In short, the difference in transverse tensile strength of the completed groove weld is governed by the reaction of the base material to the heating and cooling cycles during the welding operation.

Generally speaking, the non-heat-treatable alloys are annealed in the heat-affected zone adjacent to the weld.  This is unavoidable when arc welding, as we will reach the annealing temperature, and extended time at these temperatures is not required in order to anneal the base material.

The heat-treatable alloys are usually not fully annealed during the welding operation but are subjected to a partial anneal and overaging process.  These alloys are very susceptible to time at temperature; the higher the temperature and the longer at temperature, the more significant the loss of strength in the base material adjacent to the weld.  For this reason, it is important to control the overall heat input, preheating, and interpass temperatures when welding the heat-treatable alloys.

Typically, the common heat-treatable base alloys, such as 6061-T6, lose a substantial proportion of their mechanical strength after welding. For example, 6061-T6 typically has 45,000 PSI tensile strength prior to welding and around 27,000 PSI in the as-welded condition. One option with the heat-treatable alloys is post weld heat-treatment to return the mechanical strength to the manufactured component. If post-weld heat-treating is considered, the filler alloy’s ability to respond to the heat-treatment should be evaluated.

Most of the commonly used filler alloys will not respond to post-weld heat treatment without substantial dilution with the heat-treatable base alloy. This is not always easy to achieve and can be difficult to control consistently. For this reason, filler alloys have been developed to independently respond to heat-treatment.  

As an example, filler alloy 4643 was developed for welding 6xxx series base alloys and developing high mechanical properties in the post-weld heat-treated condition. This alloy was developed by taking the well-known alloy 4043, reducing the silicon, and adding 0.10 to 0.30 percent magnesium, thus ensuring its ability to unquestionably respond to post-weld heat-treatment.
About The Author

Tony Anderson is Corporate Technical Training Manger for ESAB North America prior to his current position he was the Technical Director for AlcoTec Wire Corporation.  He is a Senior Member of the TWI and a Registered Chartered Engineer.  He is Chairman of the Aluminum Association Technical Advisory Committee for Welding and holds numerous positions including Chairman, Vice Chairman and Member of various AWS technical committees.  Questions may be sent to Mr. Anderson via e-mail at tanderson@esab.com.